    环氧地坪涂料的效果,表面坚硬平滑、抗冲击性能好;色泽均匀、光亮、无接缝;保养方便、维修费用低,且有很好的装饰效果。一、施工材料:主要材料为无溶剂型环氧地坪涂料环氧底漆、中涂和面涂;辅助材料为金刚砂和石英粉等。

    The effect of epoxy floor coating, surface hard and smooth, good impact resistance; uniform color, bright, seamless; easy maintenance, low maintenance costs, and has a good decorative effect. 1. Construction materials: The main materials are solvent-free floor coatings epoxy primer, intermediate coatings and topcoatings; auxiliary materials are Emery and quartz powder. 二、施工工艺

    Two. Construction technology


    1.基层处理

    1. grassroots treatment


    清理打磨,用砂轮打磨机把混凝土表面的浮粒、水泥浮浆以及粘附的垃圾杂物打磨掉,清扫干净。地面缝隙用气泵吹冲至无灰尘及杂物。

    Cleaning and grinding, grinding wheel grinding machine to the concrete surface of floating particles, cement slurry and adherent garbage debris grinding, clean up. The ground gap is blown to dust and debris by air pump.


    2.混凝土缝隙处理

    2. concrete slot treatment


    缝隙表面封堵密实。配合比为5∶1加入适量的金刚砂,调成稠粥状。检测车间东半部分中间往北先处理缝隙,其他部分均为后处理缝隙。混凝土断块用切割机切成凹槽,使用柔性环氧树脂砂浆进行填塞、平整处理。

    The surface of the slit is tightly packed. Mix 5 to 1, add the right amount of emery, and make the thick porridge. Check the east half part of the workshop to deal with the gap first, and the other parts are all post-processing gaps. The concrete fault block is cut into grooves by cutting machine, and is filled and leveled by flexible epoxy resin mortar.


    3.涂刷底漆

    3. priming paint

    "

    使用无溶剂型环氧底涂漆,底涂A黄色,底涂B黑褐色,配合比A∶B=4∶1,加入适量的金刚砂。使用专用滚刷先横后竖滚刷2遍,要求滚刷均匀、无漏涂、无堆积。

    Using solvent-free epoxy primer, primer A yellow, primer B black brown, mix ratio A:B=4:1, adding appropriate amount of emery. Use the special rolling brush to brush the brush 2 times after rolling vertically and evenly.

    4.中涂砂浆

    4. medium mortar

    使用无溶剂型环氧中涂漆,按配合比5∶1混合后加适量40~100目石英砂搅拌均匀,用抹子满刮1~2遍。固化后用专用砂轮机将刮纹等打磨平整。中涂完成,严禁任何人进入。

    Use solvent-free epoxy medium coat, mix in proportion to 5:1, add appropriate amount of 40-100 mesh quartz sand to stir evenly, scrape 1-2 times with a plaster. After curing, special scratching machine is used to smooth the scratch. No one is allowed to enter.

    5.面涂打底

    5. sides applied to the bottom.


    配合比A∶B=4∶1,A为面层的色涂料,B为白色涂料,不添加任何材料,满刮一遍。周边、设备边缘使用面层涂料,用毛刷提前处理1遍。

    Mixture A:B=4:1, A is the surface color paint, B is the white paint, without adding any material, full scrape once. Use the surface coating on the periphery and equipment edge, and use the brush to deal with it 1 times in advance.

    6.涂刷面涂料

    6. brushing paint


    根据要求加入颜色,同样按配合比A∶B=4∶1,A为面层的色涂料,B为白色涂料,另外用稀料调整稠度,调完后稀稠度达到把底漆颜色盖上,且无针孔、气泡等缺陷。第1遍滚涂横刷且垂直,滚刷滚涂时横竖滚涂各1遍,把基层全部覆盖。

    According to the requirements to add color, the same mix proportion A: B = 4:1, A for the surface of the color paint, B for white paint, in addition to adjust the consistency with thinner, after adjusting the thinner consistency to the primer color cover, and no pinholes, bubbles and other defects. First times rolling and spreading horizontally and vertically, rolling and rolling, rolling and coating each other 1 times, covering all the grass-roots.


    7.耐磨层

    7. wear-resistant layer


    用环氧耐磨面漆滚涂1遍,可显著提高环氧地坪光洁度和耐磨性能。总厚度要求为3~5?mm。

    Rolling with epoxy abrasion resistant finish for 1 times can significantly improve the finish and wear resistance of the floor. The total thickness required is 3~5 mm.

    8.养护

    8. maintenance

    自然养护或喷刷养护剂,养护7?d后,方能承受重负荷。养护期间避免水或其他溶液侵入表面。

    Natural curing or spray curing agent can withstand heavy load after curing for 7 d. During maintenance, avoid water or other solution to invade the surface.

    9.验收

    9. acceptance

    温度在25℃时,2~3?d可达强度设计值的80%。用小锤敲击不空鼓;用2?m靠尺高差小于3~4?mm;用驾校货车在地面上进行刹车试验,面层无变化;接口处平整、颜色一致、无明显施工滚筒及批刀痕迹,光泽度应不小于70%。涂膜外观无针孔、无气泡、无褶皱。大面积的施工观感与试件进行比较不吸水,不粘灰。

    When the temperature is 25 degrees, the 2~3 value of D can reach 80% of the strength design value. The drum can not be knocked hollow with a small hammer; the height difference of 2_m is less than 3 ~ 4_m m; the brake test is carried out on the ground with a driving school truck, and the surface layer is unchanged; the interface is smooth, uniform in color, and there is no obvious traces of construction drum and batch knife, and the gloss should not be less than 70%. There is no pinhole, no bubbles and no wrinkles. A large area of construction is compared with the specimen without water absorption and no dust.


    三、基底混凝土缝隙缺陷、面层针孔的处理

    Three. Treatment of base concrete crevice defects and surface pinholes.


    (1)混凝土缝隙面层施工后,第2~3?d抽查,发现褶皱;第3~4?d抽查褶皱部位增高且空鼓,开始切缝,及时处理。

    (1) After the construction of concrete crevice surface layer, folds were found on the 2nd to 3rd_d spot checks, and the 3rd to 4th_d spot checks showed that the folds were increased and empty, and cracks were cut and treated in time.

    (2)面层针孔发现后,上人不粘脚时,马上用排笔补刷。

    (2) when the surface pinhole is found, when the upper person does not stick to his feet, he will use a pen to brush.